Traduccion en castellano de esta pagina
 
Back to Previous Page
 

Locus-of-Break codes for Fillet Extrusion Weld Seams Tested for Seam Strength in Shear and Peel Modes.


Type of Break Code   Break Description  

AD-1   Failure in adhesion. Specimens may
also delaminate under the bead and
break through the thin extruded
material in the outer area.
 
 
AD-2   Failure in adhesion.  
 
AD-WLD   Break through the fillet.  
 
SE-1   Break at seam edge in the bottom sheet. (Applicable to shear tests only.)  
 
SE-2   Break at seam edge in the top sheet.
(Applicable to shear tests only.)
 
 
SE-3   Break at seam edge in the bottom sheet. (Applicable to
peel tests only.)
 
 
BRK-1   Break in the bottom sheeting. A "B" in parenthe-
sis after the code means the speci-
men broke in the buffed area.
 
 
BRK-2   Break in the top sheeting. A "B" in parenthe-
sis after the code means the speci-
men broke in the buffed area.
 
 
AD-BRK   Break in the bottom sheeting after some adhe-
sion failure between the fillet and the
bottom sheet.
 
 
HT   Break at the edge of the hot tack for
specimens which could not be de-
laminated in the hot tack.
 
 
SIP   Separation in the plane of the sheet.  
(1) Acceptance of AD-Weld breaks depends on whether test values meet a minimum specification value.

 
 
Back to Previous Page
 

 
    
 search words or keywords :  

[Get  
Home Products Technical Company Info News FAQ Site Map Contact Us Español
 
Poly-Flex, Inc. • 2000 W. Marshall Dr. • Grand Prairie, TX 75051 U.S.A. • 888-765-9359
© Poly-Flex, Inc. • All Rights Reserved